Strong surface decarburization - 1.3505

Treatment :  spheroidised
Magnification :  100 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

strong surface decarburization in the form of

lamellar pearlite 0,20 mm deep

Treatment :  spheroidised
Magnification :  200 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

strong surface decarburization in the form of

lamellar pearlite 0,20 mm deep