Segregation with cementite accumulation - 1.3505

Treatment :  spheroidised (quenched for the testing)
Magnification :  50 : 1
Etching medium :  10 % alcoholic nitric acid - deep etching
Sampling / Specification :  transverse
Testing result :

core segregation with cementite lattice

and cementite accumulations

Treatment :  spheroidised (quenched for the testing)
Magnification :  50 : 1
Etching medium :  10 % alcoholic nitric acid - deep etching
Sampling / Specification :  longitudinal
Testing result :

core segregation with cementite lattice

and cementite accumulations

previous page

back to material defects

 

next page