Insufficient austenitization at the quenching - 1.2242

Treatment :  quenched and tempered
Magnification :  200 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

bad heat treated - underhardened :

mixture of ca. 50 % heat treated structure
and 50 % annealing structure

Treatment :  quenched and tempered
Magnification :  500 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

bad heat treated - underhardened :

mixture of ca. 50 % heat treated structure
and 50 % annealing structure