Treatment : quenched and tempered
Magnification : 6,5 : 1
Etching medium :
Sampling / Specification : surface - head burst
Testing result :
strong burst in the area of the upseted
screw head |
Treatment : quenched and tempered
Magnification : 100 : 1
Etching medium :
Sampling / Specification : transverse
Testing result :
rolling defect 0,23 mm deep with small slag