Scratch after grinding - 1.4104

Treatment :  annealed - ground
Magnification :  25 : 1
Etching medium :  
Sampling / Specification :  steel bar surface
Testing result :

scratch on the ground surface
going in lengthways direction

Treatment :  annealed - ground
Magnification :  50 : 1
Etching medium :  
Sampling / Specification :  transverse
Testing result :

scratch 0,03 mm deep
the edges of the defect are raised lightly
the defect has arisen after grinding

previous page

back to material defects

 

next page