Stress crack in a nitrided component - 1.8507

Treatment :  quenched and tempered - nitrided
Magnification :  50 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

stress crack arisen at the quenching
the flanks of the crack became nitrided also
the defect was already existing before the nitriding

Treatment :  quenched and tempered - nitrided
Magnification :  1000 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

basic structure
ferrite free heat treated microstructure

previous page

back to material defects

 

next page