Examinations at the material 1.2201

Treatment :  30 min. 1000° C / air
Magnification :  500 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

martensite with carbide precipitates

primary carbides
hardness : 788 HV 10 (average of 3 measurements)

Treatment :  30 min. 1000° C / air
Magnification :  1000 : 1
Etching medium :  3 % alcoholic nitric acid
Sampling / Specification :  transverse
Testing result :

martensite with carbide precipitates

primary carbides

previous page

back to examinations

back to wb2201